Rubber & Plastic Products

Natural Pigments Survive Most PLA and PBS Processing, but UV Stability Limits Use

A study of four bio-based colorants in biodegradable polyesters finds conventional compounding feasible, while lightfastness remains the main barrier.

Nadia SorensenNovember 2, 20265 min read4 views
Natural pigment powders and colored polymer strands beside PLA and PBS pellets, illustrating melt-compounded bio-based color masterbatches.

Natural colorants are often presented as a lower-impact alternative to conventional pigments, but their practical value depends on whether they can pass through the same melt-processing equipment as the polymers they color. A recent study, 'Sustainability in the Development of Natural Pigment-Based Colour Masterbatches and Their Application in Biopolymers,' examined that question for four commercial natural pigments in two biodegradable polyesters: polylactic acid (PLA) and polybutylene succinate (PBS). The results show a narrow but real processing window: most formulations could be compounded and molded on conventional equipment without large changes in flow or mechanical behavior, but color retention during processing and exposure remained uneven.

What the study tested

The researchers used blue spirulina, yellow curcumin, red beetroot, and green chlorophyllin. Each pigment was combined with PLA and PBS to make color masterbatches by twin-screw extrusion. The masterbatches also contained titanium dioxide, calcium carbonate, and stearic acid, added to support UV protection, dispersion, and processing. The masterbatches were then diluted into the matching polymer at 2, 4, and 6 wt%, and test specimens were produced by injection molding. This is a conventional route for color masterbatches, which matters because a natural color system is unlikely to be adopted if it requires a fundamentally different compounding line.

Thermal window determines compatibility

The main constraint was heat. Natural pigments are organic structures and can begin to degrade at lower temperatures than the polymers they are meant to color. Thermogravimetric analysis put the degradation onset at about 229 °C for spirulina, 244 °C for curcumin, 258 °C for chlorophyllin, and 267 °C for beetroot. PLA and PBS degrade at considerably higher temperatures, but their melting and processing requirements still differ enough to change the pigment outcome.

To limit thermal exposure, the researchers selected extrusion profiles that melted each polymer while keeping temperatures as low as practical. Processing temperatures reached 145 °C for PBS and 190 °C for PLA. The twin-screw extruder ran at 65 rpm with a feed rate of 2 kg/h. Most pigment–polymer combinations fit this window. Spirulina was the clear exception: during PLA processing it lost its characteristic blue color, so a blue PLA masterbatch could not be produced. PBS, processed at the lower 145 °C, preserved enough pigment stability for successful compounding.

That contrast is the central processing lesson. Pigment compatibility is not only a property of the colorant; it depends on the thermal profile imposed by the polymer matrix. A pigment that works in PBS may fail in PLA even when both are processed below the pigment’s measured onset temperature. The reported results do not identify the exact degradation mechanism, but the practical outcome is clear: the blue colorant could not survive the higher-temperature PLA route in this formulation.

Flow and mechanical effects are limited

From a compounding perspective, the natural pigments caused only limited changes in rheology. Melt flow rate decreased slightly after pigment incorporation, indicating a modest increase in melt viscosity. Neat PLA had an MFR of about 50 g/10 min, and the natural-pigment masterbatches stayed close to that value. PBS showed a similar response, with only a minor reduction in melt flow rate.

That matters for scale-up. A color system offers little practical value if it forces major changes to screw design, pressure settings, or molding conditions. In this study, conventional twin-screw compounding and injection molding handled most formulations without major processing problems. The window was not universal, but it was compatible with standard equipment.

The researchers also checked tensile and impact behavior across the 2 to 6 wt% addition range. Neither PLA nor PBS showed significant losses in overall mechanical performance. PLA started with a Young’s modulus of about 1710 MPa and tensile strength of 65.6 MPa; PBS started at about 392 MPa and 34.5 MPa. The colored formulations stayed close to those baselines. Impact strength also remained in a similar range, although individual pigments produced some variation. These results support the view that, at the tested loadings, the pigments did not fundamentally disrupt the polymer matrices.

UV stability remains the weak point

Successful extrusion did not ensure long-term color stability. After 50 hours of xenon-lamp exposure, most formulations showed a color difference above ΔE* = 2, a level generally considered visually perceptible. The PLA formulation containing 2 wt% green chlorophyllin masterbatch had the highest photostability and remained the main exception.

The study therefore identifies UV stability as the largest barrier to broader use. Packaging, consumer products, agricultural parts, and outdoor applications may need additional stabilization, protective coatings, or pigment modification before natural colors can compete with conventional systems over long service periods. The processing results show that natural pigments can be incorporated; the durability results show that incorporation alone is not enough.

Environmental gain versus performance gap

The environmental comparison favored the natural pigments under the study’s assumptions. One kilogram of curcumin pigment generated about 0.04 kg CO2-eq, compared with 18.65 kg CO2-eq for the inorganic green reference pigment. The natural-pigment masterbatches also consumed less electricity during extrusion and pelletizing. Those figures are important because they indicate a potential footprint advantage at the colorant and compounding stages, not merely a marketing claim about bio-based origins.

That advantage must still be weighed against performance. The study notes that packaging, consumer, agricultural, and outdoor applications may require additional stabilization, protective coatings, or pigment modification; it does not quantify how those extra steps would affect the footprint comparison. The CO2 figures should therefore be read as an indicator for the pigment and selected processing steps rather than a complete verdict on the final application.

What the results mean

The work demonstrates that several natural colorants can be compounded into PLA and PBS using conventional processing equipment, with only limited changes in melt viscosity and mechanical performance. It also shows that thermal compatibility is matrix-specific and that spirulina is not a drop-in blue for PLA under the reported conditions. The largest remaining development need is color stability, both during processing and during subsequent service exposure.

For compounders and product developers, the implication is practical: natural pigments are technically viable in these biopolymers, but they should be selected against the actual polymer’s processing temperature and the intended service environment. The results suggest that applications able to accept additional stabilization or protective measures are closer to practical use than long-life outdoor products. Further work on lightfastness, thermal stability, and pigment modification will determine whether these colorants move from promising formulations to routine commercial options.